Views: A stainless steel oxygen line comes back from degreasing with a bright, clean bore that passes visual inspection. Under a UV lamp the flange face glows yellow-green, and the line is rejected. The problem is that grease leaves no colour, no texture and no smell: in white light a well-cleaned surface and a nearly cleaned one look identical. This article covers why pure oxygen systems must be degreased, which documents set the requirements, how to choose among four degreasing methods and three chemical families, and the standard process flow. It then compares the resolution of four acceptance tests and explains why the UV fluorescence check is the step where acceptance usually stalls, with reference to inspection lamps such as the LUYOR-2130L.
A stainless steel oxygen line: degreasing and cleaning are finished, the bore has been wiped until it shines, and visual inspection finds nothing to object to. Then, at acceptance, a UV lamp is switched on and the flange face glows yellow-green - rejected, rework.
This is a familiar scene on site. The problem is not the cleaning process but what cannot be seen: grease residue does not change the colour of the metal, does not change its surface finish and produces no smell. Under ordinary white light, "washed thoroughly" and "almost there" look exactly the same. Nothing but a UV lamp at 320-380 nm will show the difference.
This article avoids generalities and deals with three things that actually stop work on site: why the pipe must be degreased, how the degreasing is done, and why the UV lamp method is the one that can check every surface at acceptance; along the way it sets out the figures a degreasing inspection blacklight has to meet to be usable for acceptance, and how the LUYOR-2130L is used on real oxygen line projects: how to work it, how to judge, how to keep the record.
Oxygen-wetted parts must be degreased because pure oxygen supports combustion: grease residue is an ignition hazard the eye cannot see, not a question of whether the part looks dirty.
HG 20202 lists four test methods. Of these, the UV lamp method is the one that combines on-site working, an immediate result, full coverage, a photographic record and no damage to the part.
A lamp used for acceptance has to meet three hard figures: centre intensity, effective spot and white light level; a lamp that is not bright enough, or whose spot is too small, produces a false pass.
The LUYOR-2130L is a wide-area model with three 365 nm UV-A LEDs: about 25000 μW/cm² at 150 mm, a spot of about 100 mm and white light below 15 lux.
The key actions on site are "far, then near" and "wipe once": scan the whole area from a distance, confirm points up close; most of what wipes away is fibre and dust, and what does not wipe away is grease.
Start with the principle, because it decides why every later check has to be that strict.
Oxygen does not itself burn, but it is a strong oxidiser and supports combustion. In air at room temperature iron and copper are "non-flammable" materials; in pure oxygen they both burn steadily. Grease left on the bore is energised by the high-velocity oxygen stream and by impact from solid particles, and heats up locally; once the temperature passes the ignition point the pipe wall itself ignites, and pure oxygen makes the fire burn harder, concentrating heat until the wall burns through and the system explodes.
Risk therefore follows three variables: the purer the oxygen, the greater the hazard (high-purity oxygen is far more hazardous than oxygen-enriched air), the higher the pressure and velocity, the greater the hazard, the smaller the bore and the sharper the throttling, the greater the hazard (the same flow runs faster in a small pipe and at an elbow). This explains why the oxygen lines of a gasification unit, the inlet and outlet of an oxygen compressor in an air separation plant, and medical central oxygen piping are all locations with strict degreasing requirements.
The cases below normally need degreasing and acceptance testing as soon as the medium touches oxygen:
| Case | Typical objects | Why degrease |
|---|---|---|
| Air separation and industrial gases | Oxygen lines in cryogenic air separation plants, oxygen compressor piping, liquid oxygen tanks and lines | Oxygen purity is very high, so any grease residue is an ignition source |
| Medical gas engineering | Hospital central oxygen piping, manifolds, pressure regulators, terminals | Occupied buildings, the highest safety class, with gas purity also specified |
| Chemical and energy | Oxygen lines in coal gasification units, hydrogen and liquid oxygen systems | High pressure, high flow, many throttling points, concentrated risk |
| Equipment and test rigs | Liquid oxygen systems, high-pressure oxygen test benches, oxygen valves and instruments | Frequent starts and stops, extreme conditions, demanding cleanliness |
Table 1 Typical cases that need degreasing and acceptance (all oxygen-wetted surfaces)
| Document | Covers | Relation to this topic |
|---|---|---|
| Degreasing Engineering Construction and Acceptance Specification, HG 20202 | Degreasing work and acceptance | Gives four test methods, including UV lamp inspection, with pass criteria; the direct basis for this work |
| Safety Technical Code for the Production of Oxygen and Related Gases by Deep Cooling, GB 16912 | Oxygen production and use safety | Requires oxygen-wetted parts to be degreased and stresses preventing recontamination afterwards |
| Code for Construction of Industrial Metallic Piping, GB 50235 | Industrial metallic piping construction | Sets cleanliness requirements and inspection steps for oxygen piping |
| Technical Conditions for Valves for Oxygen Service, GB/T 12244 | Oxygen valves | Sets limits for grease residue in valve bodies and on sealing faces (≤125 mg/m² is commonly quoted) |
| ASTM G93-96 (common on export projects) | Oxygen system cleanliness | The usual criterion is surface oil content below 1 g/m² |
Table 2 The chain of standards relevant to degreasing. Names and editions follow the project design documents, tender documents and contract.
1 g/m². What does 1 g/m² mean? Roughly less than half a drop of oil spread evenly over the area of an A4 sheet. A residue that small is still a hazard that has to be removed, which is why degreasing cannot be judged by "it looks clean".Understand the process and you can see, at acceptance, where problems are likely to arise. Degreasing comes down to three things: which method, which chemical, in which order.
| Method | Applies to | Advantages | Limits |
|---|---|---|---|
| Immersion (tank) | Removable pipe spools, flanges, valves, gaskets, fasteners | Full coverage of internal surfaces, even result, batch handling | Needs a degreasing tank and space; unsuitable for very long spools or installed lines |
| Wiping / swabbing | Valve bodies, isolated spots and pipe ends that cannot be immersed | Flexible, local treatment, simple tools | Slow, and the result depends on how careful the operator is; fabric fibres are easily left behind |
| Circulation (forced circulation) | Long installed lines, large-diameter mains | Covers the whole system in one pass, uniform result, less labour | Needs a cleaning pump skid and a temporary loop; a large amount of preparation |
| Spraying | Vessel internals, large-diameter sections | Large coverage, handles big cavities | Needs dedicated equipment; spray shadows remain |
Table 3 Where the four common degreasing methods apply and where they do not
One line on selection: use immersion for prefabricated spools wherever possible, because the result is even; for long lines already installed, circulation is less labour and more reliable than wiping each section repeatedly, because it gives every section and every component the same treatment, while hand wiping varies from crew to crew.
Organic solvents (carbon tetrachloride, trichloroethylene, acetone and similar): strong degreasing power, usable at room temperature. Note carefully: carbon tetrachloride is toxic, volatile and a controlled substance; use it with an inhibitor, never with water present, and with strict ventilation and personal protection. Many projects now move to alternatives where they can.
Water-based alkaline (for example 3-5% sodium hydroxide, steam-heated to about 80℃ for immersion): low cost, easy waste treatment, reusable, and widely used. Watch compatibility with aluminium and similar materials, and rinse thoroughly to neutral after degreasing.
Water-based neutral / emulsifying (emulsifying degreasers containing surfactants): mild, kind to the substrate, suited to situations where strong alkali cannot be used.
Acid cleaning removes rust and welding slag; passivation grows a dense protective film so the steel does not rust again after degreasing; the cleanliness check is the degreasing inspection this article is about. Once the flow is finished, a pipe that passes should be passivated or closed off with dry nitrogen as soon as possible to prevent recontamination - much of the rework comes from a pipe that was soiled again after it had already passed.
HG 20202 gives four usable test methods; a project usually chooses one, and they can corroborate each other. On a construction site, however, their practicality differs enormously.
| Method | How it is done | Pass criterion | Full coverage | Record |
|---|---|---|---|---|
| UV lamp inspection | Illuminate the degreased surface with a UV source at 3200-3800 angstrom (320-380 nm) | No violet-blue (often yellow-green on site) fluorescence on the surface | Yes, suitable for full inspection | Can be photographed for the record |
| White filter paper wipe | Wipe the degreased surface with clean, dry white filter paper | No grease mark on the paper | Covers reachable areas | The paper can be kept |
| Camphor test | Blow off with oil-free steam and drop a pure camphor grain no larger than 1 mm across into the condensate | The camphor grain keeps rotating | Not suitable for full inspection | Written record |
| Analysis | Sample and analyse the degreasing bath or the surface oil content | Common criteria: oil content of the bath ≤350 mg/L; surface residue ≤125 mg/m² | Not suitable for full inspection | Produces a laboratory report |
Table 4 The four degreasing test methods compared. Criteria and limits follow the specification clauses and design documents applicable to the project.
A pipe too narrow for the lamp head is a problem every site meets. The usual practice is to wipe the bore repeatedly with a clean, oil-free non-woven cloth or white cloth, then take the cloth into the dark and illuminate it with a blacklight. No fluorescence on the cloth means that section passes; fluorescent spots mean grease is still on the bore and the section has to be degreased again.
"Buying a UV lamp" and "buying a degreasing inspection blacklight that can be used for acceptance" are two different things. The decision rests on three figures that can be measured.
The thinner the grease residue, the weaker its fluorescence under UV. Whether weak fluorescence can be excited at all depends directly on the UV intensity reaching the surface. A lamp that is not strong enough still looks violet to the eye, but a thin oil film does not fluoresce, and the operator concludes that the surface is clean. This is the dangerous failure mode in degreasing inspection: the surface is signed off as passing when the lamp simply could not reveal it, what is usually called a false pass.
Many of the places to be checked on piping are lines and rings: a flange face is a full circle, a pipe end is a circle, a weld is a line. With a small spot you have to move inch by inch, which is slow and easily skips a patch; with a large enough spot, one or two passes cover a flange. For full inspection over large areas the lamp has to be wide enough.
The value of a blacklight is that it emits UV and little visible light. If the lamp also pours out white light, weak fluorescence is drowned and the eye cannot separate it. A good degreasing inspection lamp uses an efficient filter to push the white light down; in a dark environment the contrast is higher and the eyes tire less over a long inspection.
Inspecting oxygen lines often means climbing, entering vessels and working point by point. A conventional high-pressure mercury lamp needs about 5 minutes of warm-up, its bulb surface reaches 200-300℃, and frequent switching shortens its life noticeably. On a site where you keep moving, all three cost real time. A UV-A LED is a cold source that starts instantly and can be switched at will, which makes a clear difference in use.
| Item | Ordinary UV torch / banknote checker | Conventional high-pressure mercury blacklight | LUYOR-2130L (UV-A LED) |
|---|---|---|---|
| Wavelength | Often 395 nm or a mixed band | Mainly 365 nm | 365 nm, 360-370 nm band, pure UVA |
| White light control | Mostly unfiltered, much white light | Filtered | Efficient filter, cuts over 90% of white light, below 15 lux at 150 mm |
| Start-up | Instant | About 5 minutes warm-up | Instant, full brightness |
| Frequent switching | Possible | Not advised | Possible, three levels on a touch switch |
| Surface temperature | Low | 200-300℃ | Low (aviation aluminium body dissipates heat) |
| Source life | Several thousand hours | Hundreds to several thousand hours | About 50000 hours |
| Role | General lighting / entertainment | Early degreasing inspection | On-site degreasing inspection and acceptance |
Table 5 Three common UV sources compared
The LUYOR-2130L is a torch-style blacklight from LUYOR for large-area degreasing inspection. Its design choices map onto the three figures in the previous section.
The head carries three high-power UV-A LEDs with a centre wavelength of 365 nm in the 360-370 nm band, pure UVA with no UVB or UVC. Three side by side are there to deliver enough intensity and enough spot.
It lights a surface, not a point. The effective spot is about 100 mm across at 150 mm from the head, so a flange face can be covered in one or two passes.
The filter cuts over 90% of white light, and white light at 150 mm is below 15 lux. In a dark environment the contrast is high and even a faint residue is visible.
Three more details that matter on site: Three brightness levels are switched with a touch switch at the tail, which carries a digital battery display so you do not have to guess how much charge is left; the body is hard-anodised aviation aluminium, which sheds heat quickly, and the unit weighs about 600 g with batteries, so long hand-held sessions are not tiring; the standard package includes LUV-10 UV safety glasses, a high-capacity lithium battery pack, a 110-260 V wide-range charger and an aluminium carry case, with a 3-year warranty on the unit. It is the current model, following the LPX-365 (discontinued in 2014) and the LUYOR-2130 (discontinued in 2016).
Three points matter when reading this set of figures:
Intensity falls quickly with distance. Double the distance and the intensity drops to roughly a quarter. So "can I see it" is a question of how far away you stand rather than of how much the lamp cost.
Spot and intensity trade off. Farther away shows a wider area but a shallower one; closer shows detail but a narrow band. You cannot have both at once.
The method therefore runs "far, then near". Start at the middle or low level and scan the whole surface from 250-380 mm; where a suspect bright spot appears, switch to high and move in to about 150 mm to confirm.
Compressed into an executable sequence, all of the above becomes the seven steps below.
Bring the light on site down as low as possible, screening a local area with blackout cloth where needed; check ventilation; put on the LUV-10 UV safety glasses from the kit; have oil-free white cloth or non-woven cloth, a record sheet and a pen ready.
By pipe spool number, list the bore, flange faces, welds and heat-affected zones, threaded joints, elbows and tees, valve bodies and seats, gaskets, heads, and every connection that was opened before installation.
Fix the brightness level (middle, for consistency) and the scanning distance (250 mm, for example). Using one set of conditions before and after makes comparison, repeatability and independent re-checking possible.
Work along the pipe, section by section, with the spots of successive passes slightly overlapping so nothing is skipped. Look at the whole from a distance and move quickly along the run.
Switch to high, move in to 150 mm, illuminate as square to the surface as possible and look from several angles. Wipe with oil-free white cloth and look again where necessary.
Record line by line as "spool - location - conclusion - inspector - date", and photograph anything suspect. The record itself is part of the acceptance documentation.
Degrease and re-check any location that failed; once a whole section passes, passivate it or close the ends with dry nitrogen straight away to prevent recontamination.
Flange faces: hold the head square to the face and illuminate in 3-4 passes around the circle so the full ring is covered with no gap.
Pipe-end bores: push the head slightly into the end and angle it towards the bore, keeping your own shadow out of the way.
Vessel and tank internals: run the body close to the wall in an S pattern; corners and the far end need a separate closer pass, since these are the places easily missed.
Small-bore pipe: switch to the cloth method - wipe the bore with oil-free white cloth and illuminate the cloth.
Valve bodies: dismantle the valve and inspect one by one; the seat and sealing face matter most, because grease there is easily hidden once the valve is assembled.
The pass criterion for UV lamp inspection is simple: no violet-blue (often yellow-green on site) fluorescence on the surface. The difficulty on site is separating the fluorescence of grease from the fluorescence of everything else.
| Interference | Fluorescence signature | How to tell |
|---|---|---|
| Cotton and fabric fibres | Thin filaments, drawn out, bright blue-white | Wipe with oil-free white cloth and it comes away |
| Dust and paper fragments | Scattered points, sharp boundary | Blow off or wipe away |
| Residue of some cleaners or degreasers | In patches, even, following the cleaning path | One more rinse and it disappears |
| Rust-preventive oil / cutting fluid / marker ink | Spots and lines with a definite direction | Still there after wiping; degrease again |
| Sealant, coating, label adhesive | Local patches with clear boundaries | Check against the process step; do not misread it |
| Hand sweat / skin oil | Fingerprint shaped | Change gloves and look again |
Table 6 Common interference that fluoresces under UV but is not grease residue
Form adds another clue: drawn out lengthwise, with blurred edges and running into bands is usually the mark left by fabric fibre rubbing; spots with sharp edges, fixed on a sealing face or a weld are usually genuine grease residue.
Every UV source loses output with use, LEDs included, though far more slowly. In degreasing inspection this matters: once a lamp has decayed far enough, residual oil stops showing and the inspection turns into a false pass - which is more dangerous than no inspection at all, because it produces a wrong release decision.
Two controls are worth putting in place:
Fix the distance and the brightness level, measure centre intensity with a UV meter at intervals, and enter it in the equipment log. A lamp is a measuring instrument and should have one.
For example, send the lamp for service or replace the source when centre intensity falls below 70% of its initial value. Put the threshold in the work instruction so the decision does not rest on how someone feels.
Meters that go with it: the LUYOR-340 UV meter, and UV radiometers from Spectroline and other brands. We can supply a measurement and logging scheme that fits your existing record format.
Degreasing inspection is not one single situation, so one lamp does not cover everything. Split by "surface or point, and whether a report is needed", the division of work looks roughly like this:
| Model | Beam type | Key data | Better for |
|---|---|---|---|
| LUYOR-2130L | Wide area (3 LEDs) | About 25000 μW/cm² at 150 mm, spot about 100 mm, white light <15 lux | Full degreasing inspection of oxygen lines and vessels; a flange ring in one pass |
| LUYOR-3180 | Spotlight | 30000-40000 μW/cm² at 38 cm, centre beam about 30 mm | Point fluorescence: leaks, fingerprints, fine cracks; reaches farther |
| MNT-365A | Cleanroom | Smooth, low-particle body | Particle and biofilm inspection in cleanrooms |
Table 7 Selection by task
One line to remember: 2130L for a surface, 3180 for a point;
References
The cleaning acceptance standards and specification clauses mentioned here can all be traced; check the originals against the official publications below:
This article belongs to the fluorescence inspection section.
Other sections on the same product line include laboratory UV lamps (254 / 302 / 365nm single-tube and dual-wavelength benchtop lamps), 365nm blacklights (UV area lamps for NDT, leak detection and fluorescence inspection, judged by irradiance rather than wattage), life science instruments (the entry point for fluorescence imaging, UV crosslinking, UV transmission and cell irradiation).
Models mentioned in this article: LUYOR-2130L, LUYOR-340, LUYOR-3180. Ranges, accuracy and accessory lists for each model are listed on the product pages.
Email: info@xinysun.com
Tel: 131-2093-6518
Address: 1525 Minqiang Road, Bldg 26, Songjiang, Shanghai