Views: What does the OC marking for oil-free degreasing on a drawing actually require, how is the degreasing carried out, and to which standards is it accepted? Those three questions form one continuous chain of work: understand the requirement, decide the cleaning method, then know how to prove the part is clean. This article unpacks the quantitative criteria for OC, the surfaces that have to be treated, four degreasing methods and three families of chemicals, and explains the UV check at the acceptance step, including which fluorescence is oil and which is not.
People working on oxygen piping, air separation plants and medical gas projects are regularly stopped by three questions: what the "oil-free degreasing OC" note on the drawing actually means, which treatment methods exist, and to which standards the work is accepted. Taken together these three form a complete chain of work: understand what is required, decide how to clean, then know how to prove that the cleaning worked. This article follows that order and explains the role of the LUYOR-2130L degreasing inspection black light in the closing link of the chain - acceptance.
"Oil-free" is the requirement, "degreasing" is the process, and "OC" is the delivery state. The three describe one thing at three levels, and they are often used interchangeably when technical requirements are written, which leads to different readings on site.
| Term | Meaning | Where it lands |
|---|---|---|
| Oil-free | Oil-type substances are not permitted to contact the component or system; a management and design constraint | Technical conditions, drawing notes, packaging and storage requirements, assembly and pressure test rules |
| Degreasing | The construction step of removing surface grease with solvent, alkaline solution or emulsifier | Construction plan, process handover, cleaning process card |
| OC (Oxygen Clean) | The acceptance conclusion for an oxygen-clean state, meaning the part has reached a cleanliness suitable for oxygen contact | Inspection records, pass labels, handover documentation |
So the full reading of "oil-free degreasing OC" is: this is an oil-free part, it must be degreased, and it must meet the oxygen clean (OC) acceptance requirement. It is not an optional cleaning step but a mandatory requirement tied directly to safety.
Oxygen itself does not burn, but it is a strong oxidizer. In air at atmospheric pressure, steel and copper do not burn; in a pure oxygen environment they can burn continuously. Grease left on the inner wall of a pipe is energized and heated by high-velocity flow and particle impact, and once it passes the ignition point the metal of the wall ignites; the pure oxygen then feeds the fire, which can burn through the wall and lead to deflagration of the system.
Risk scales with three variables: the higher the oxygen purity, the greater the hazard, the higher the pressure and flow velocity, the greater the hazard, and the more severe the throttling, the greater the hazard (velocity is higher at elbows, tees and valves). This explains why degreasing requirements are particularly strict for oxygen lines in cryogenic air separation plants, the inlet and outlet of oxygen compressors, oxygen branch lines in gasification units, and medical central oxygen pipelines.
"Clean" cannot rest on impression; engineering uses measurable residual limits. Two criteria are often cited:
ASTM G93-96: oxygen system cleanliness is commonly judged by a surface oil content below 1 g/m². One gram per square meter is roughly less than half a drop of oil spread thinly over the area of an A4 sheet.
GB/T 12244-2021 "Valves for oxygen service - Technical specification": residual grease on the valve bore and sealing faces is commonly required to be no more than 125 mg/m², and the valve must be dried after degreasing.
The specific limit is governed by the project design documents, tender documents and contract - values differ between industries and pressure classes.
On the principle of full coverage of wetted surfaces, every internal surface that can contact oxygen is in scope: pipe and fitting bores, flange sealing faces, welds and heat-affected zones, threaded joints, elbow and tee bores, valve bores and seat sealing faces, gaskets, blind plates, tank and vessel heads, and every connection opened before installation. Pipe exteriors, supports and structural parts that do not contact the medium are usually outside the degreasing scope.
Methods divide into two layers: how to clean and what to clean with. They are chosen separately, because the same chemical behaves very differently under different methods.
| Method | Suitable for | Advantages | Limitations |
|---|---|---|---|
| Immersion (tank) method | Removable pipe sections, flanges, valves, gaskets, fasteners | Full coverage of internal surfaces, even result, batch processing | Requires a degreasing tank and floor space; unsuitable for very long sections or lines already installed |
| Wipe / swab method | Valve bodies that cannot be immersed, scattered areas, pipe ends | Flexible, allows local treatment, simple tooling | Low efficiency, result depends on how carefully the work is done; fabric fibers are easily left behind |
| Circulation (forced circulation) method | Long lines already installed, large-diameter mains | Covers the whole system in one pass, uniform result along the run, saves labor | Needs a cleaning pump station and temporary loop, and heavy preparation |
| Spray method | Vessel interiors, large-diameter pipe sections | Large coverage, can treat big cavities | Needs dedicated equipment, and spray shadows remain |
One line on selection: if a prefabricated section can be immersed, immerse it for an even result; for a long line already installed, use circulation, which is less labor and more reliable than wiping section by section - manual wiping tends to give different results from one crew to the next.
| Type | Examples | Advantages | Cautions |
|---|---|---|---|
| Organic solvents | Trichloroethylene, acetone and similar; carbon tetrachloride is now largely restricted | Strong degreasing power, works at room temperature | Toxicity, volatility and controlled-substance issues are prominent; strict ventilation and personal protection are required, and no water carry-over is allowed |
| Water-based alkaline | 3-5% sodium hydroxide solution, steam-heated to about 80℃ | Low cost, easy wastewater treatment, can be reused | Check compatibility with aluminium and similar materials; rinse to neutral after degreasing |
| Water-based neutral / emulsifying | Emulsifying degreasers containing surfactants | Mild, friendly to the substrate | Suited where strong alkali cannot be used; degreasing power has to be verified against the soil level |
Two requirements are easily overlooked: a degreaser can itself carry oil, so solvent with oil content above the limit must be de-oiled and inspected before use; and a degreased pipe must not be pressure-tested or purged with an oil-containing medium, or the earlier work is wasted. GB 16912-2008 requires oxygen piping to be purged with oil-free dry air or nitrogen after degreasing, and prohibits chlorine-containing degreasers.
The sequence usual for oxygen piping is:
Water rinse / system pressure test → degreasing → water rinse → acid cleaning → water rinse → second degreasing → water rinse → passivation → cleanliness check → oil-free air or nitrogen purge and dry
Acid cleaning removes rust and welding slag, passivation forms a protective film on the metal surface so that rust does not return after degreasing, and the cleanliness check at the end is the acceptance step covered in section 3. Once the sequence has been completed and the check passed, the part should be passivated at once or have its openings closed with dry nitrogen - a good deal of rework comes from a part that passed the check and then got dirty again.
The requirement is not aimed at oxygen alone. Any medium system that is sensitive to oil carries similar rules: high-purity gas (nitrogen, argon, hydrogen) piping, vacuum systems, refrigeration and cryogenic systems, hydrogen energy and liquid oxygen systems, and some semiconductor and precision instrument gas lines. The test is simple - if contamination of the medium by grease would affect safety, purity or function, the part should be managed as an oil-free part.
| Standard | What it covers | Relation to this topic |
|---|---|---|
| HG 20202-2000 "Code for construction and acceptance of degreasing works" | Degreasing construction and acceptance | The dedicated degreasing standard. Gives inspection methods such as UV lamp examination and the criterion "no violet-blue fluorescence means acceptable" |
| GB 16912-2008 "Safety technical regulations for the production of oxygen and related gases by deep freezing" | Safety of oxygen production and use | Requires oxygen-contact parts to be degreased, purged with oil-free dry air or nitrogen after degreasing, and prohibits chlorine-containing degreasers |
| GB 50235-2010 "Code for construction of industrial metallic piping" | Industrial metallic piping construction | Sets cleanliness requirements for oxygen piping and the pre-installation inspection step |
| GB/T 12244-2021 "Valves for oxygen service - Technical specification" | Oxygen valves | Sets limits on residual grease in the valve bore and on sealing faces |
| GB 50751-2012 "Technical code for medical gas engineering" | Medical gas systems | Sets cleanliness and inspection requirements for medical gas piping, terminals and manifolds |
| ASTM G93-96 | Oxygen system cleanliness | Often used on projects with an international scope; the criterion is usually a surface oil content below 1 g/m² |
This is a table that gets asked about often. The four methods differ widely in how practical they are:
| Method | How it is done | Pass criterion | Full inspection possible | Evidence retained |
|---|---|---|---|---|
| UV lamp examination | Irradiate the degreased surface with a UV source at 3200-3800 Å (that is 320-380 nm) | No violet-blue (often yellow-green on site) fluorescence on the surface | Yes | Can be photographed for the file |
| White filter paper wipe | Wipe the degreased surface with clean, dry white filter paper | No grease trace on the paper | Where the paper reaches | The filter paper can be kept |
| Camphor method | Blow off with oil-free steam and place the condensate around pure camphor no larger than 1 mm in diameter | The camphor particle keeps rotating | Not suited to full inspection | Requires a written record |
| Analytical method | Sample and analyse the grease content of the degreasing bath or of the surface | Common criteria: grease content of the bath ≤350 mg/L; surface residue ≤125 mg/m² | Not suited to full inspection | Laboratory report issued |
The specification requires the inspection quantity for degreased parts to be all of them, with degreasing and inspection records retained. In other words, every flange and every weld has to be looked at. UV lamp examination is the method that satisfies five conditions at once: it can be done on site, it gives a result immediately, it covers every location, it leaves an image record, and it does not damage the part. The filter paper and camphor methods suit re-checking a suspect area, and the analytical method suits quantitative spot checks and issuing a report.
About the "3200-3800" in the standard: the original unit is the angstrom (Å), 1 Å = 0.1 nm, so the conversion gives 320-380 nm, squarely inside the UV-A band. That is why degreasing inspection lamps are always 365 nm and not 254 nm - when buying a lamp, if the word on offer is just "ultraviolet", confirm that the wavelength falls in the 320-380 nm range.
Cleaning and checking are two different things. The cleaning side depends on process and chemicals; the checking side needs a lamp that can reveal weak fluorescence and still cover a whole flange circumference and a pipe end. The LUYOR-2130L is designed around this "full inspection" requirement.
| Requirement that full inspection imposes | Corresponding design of the LUYOR-2130L |
|---|---|
| Wavelength must fall in 320-380 nm | 3 × high-power 365 nm UV-A LEDs, band 360-370 nm, pure UVA without UVB or UVC |
| The spot has to be large enough for fast coverage | Spot about 100 mm at 150 mm, about 150 mm at 250 mm, about 200 mm at 300 mm |
| Intensity has to be high enough for thin oil films to fluoresce | About 25000 μW/cm² at 150 mm; about 13000 μW/cm² at 250 mm; about 10000 μW/cm² at 300 mm |
| White light has to be suppressed for fluorescence to be readable | High-efficiency filter cuts more than 90% of white light; white-light illuminance at 150 mm below 15 lux |
| Must switch on and off often and move easily | UV-A LED cold source lights instantly, three brightness levels on a light touch; body 220 mm long, reaches into pipe ends |
| Must enter tight spaces | Flashlight form, head 76 mm, tail 45 mm, net weight about 600 g |
| Working time has to be sufficient | Lithium battery, about 2-5 hours of continuous operation depending on the level |
| Battery state has to be visible | Digital battery display at the tail of the body, so the lamp does not die halfway through |
UV intensity falls quickly with distance, so intensity figures always have to be read together with distance: from 150 mm out to 380 mm the center intensity drops to roughly a quarter. The usual site practice is "far then near" - sweep quickly at 250-380 mm on the middle and low levels to find suspect areas, then switch to the high level and move in to about 150 mm to confirm detail.
The pass criterion is no violet-blue fluorescence on the inspected surface. Note "none", not "very weak" - there is no intermediate grade of "slightly acceptable" in this reading.
| Interference that fluoresces but is not grease | Source | How to tell it from grease |
|---|---|---|
| Cotton fibers, lint from cleanroom wipes | Shed during wiping, carried on clothing | Wipes off with an oil-free white cloth; filamentous or dotted in form |
| Dust and inorganic particles | Airborne dust, concurrent trades | Removed by wiping; grease spreads into a halo |
| Cleaning agent and degreaser residue | Incomplete rinsing | Re-rinse and dry per the process, then re-check; do not rush to fail the part |
| Rust-preventive oil, protective wax | Factory protective layer not fully removed | Sheet-like distribution with regular edges; this is "not degreased" rather than "poorly degreased" |
| Marker pen strokes, label adhesive | Construction marking | Fixed position, regular shape, obvious at a glance |
One action that works better on site than any theory: wipe it. Rub an oil-free white cloth gently over the suspect bright spot - what comes off is mostly foreign fiber and dust; what stays, or still shows a yellow-green halo after wiping, is grease that has seeped into microscopic surface depressions. Writing this action into the work instruction is recommended.
Broadly synonymous, but OC puts more weight on the delivery state of "inspected against the oxygen clean requirement, with records kept". OC is the clearer term in a technical requirement, because it implies that acceptance was performed, records exist and the part is labelled.
Common industry practice: wipe the bore repeatedly with a clean, oil-free non-woven or white cloth, then take the cloth into a dark area and examine it under a black light. If the cloth shows no fluorescence, that section passes; fluorescence spots mean it has to be degreased again. This is the HG 20202 white filter paper method and UV lamp method applied together.
Yes, and strongly. The more visible ambient light there is, the less a weak fluorescence can be seen. Where conditions allow, screen the area with a light-blocking cloth or work in a dark room; if the shop lighting cannot be switched off, hood the inspection area and look inside. Judging "pass" directly may in fact mean nothing more than that nothing was visible.
No. UV intensity falls as the source ages, and past a certain point the fluorescence of a thin oil film can no longer be seen, so inspections "pass" smoothly until a problem appears at charging or pressure testing. The basis for judgement should be intensity data with records and a threshold: fix the level and the measuring distance (high level at 250 mm, for example), measure the center intensity under the same conditions each time and log it in the equipment file, and set a replacement threshold (for example below 70% of the initial value, send for calibration or replace). A UV radiometer can be used for this work.
Not advisable. The usual problems are a wavelength shifted to 395 nm, no filter so too much white light, a small spot and insufficient intensity. Those three map exactly onto "no fluorescence visible", "fluorescence drowned by white light" and "a small spot that misses areas", and the outcome is a false pass. A lamp used for acceptance has to meet four points: 320-380 nm wavelength, sufficient center intensity, low white-light illuminance and a large enough spot.
The test is simple: is your main worry incomplete coverage or an unclear view. Degreasing inspection of oxygen piping covers a large area and requires every location to be seen, so what you fear is a miss - take the widely distributing 2130L; fluorescent leak detection and penetrant inspection look for very small points, so what you fear is not seeing them - take a focusing high-intensity type such as the LUYOR-3180. Many organizations working on oxygen piping keep both: one for finding, one for sweeping.
Back to the three questions at the start. Oil-free degreasing OC is the combined name for "oil-free part + degreasing treatment + oxygen clean acceptance", and the criterion is a measurable limit on residual surface grease; treatment methods mean four methods with three families of chemicals, worked through the process chain before acceptance; standards start from HG 20202 as the dedicated degreasing basis and link with GB 16912, GB 50235 and GB/T 12244, with ASTM G93 often cited on projects with an international scope.
One link in that chain is especially prone to looking done when it is not: the acceptance step at the end. Grease residue does not change the color of the metal, does not change its finish and produces no smell. Making it visible takes a 365 nm lamp with the right wavelength, enough intensity, a large spot and low white light.
If a project needs the selection for a degreasing inspection plan checked (pipe diameter, locations, working time), or needs a recording scheme for UV intensity verification, send us the working conditions and we will confirm them together. Further reading: Why pipe degreasing is accepted under UV light, 365nm black light section, UV radiometer section.
This article belongs to the frequently asked questions section.
Other sections on the same product line include 365nm black lights (UV surface sources for penetrant inspection, leak detection and fluorescence checks, where irradiance matters more than wattage), surface inspection lamps (low-angle grazing light that pulls particles, scratches and fingerprints out of the background) and industrial test instruments (the entry point for UV inspection, rotational speed measurement, stroboscopic observation and surface inspection).
Models mentioned in this article: LUYOR-3103, LUYOR-BBMA, LUYOR-365L. Ranges, accuracy and accessory lists for each model are listed on the product page.
Email: info@xinysun.com
Tel: 131-2093-6518
Address: 1525 Minqiang Road, Bldg 26, Songjiang, Shanghai
Copyright 2026 Xinysun Instrument (Shanghai) Co., Ltd. All rights reserved.
ICP:ICP-2026046447